Although several alloys from some immiscible elements such as Fe/Cu, F
e/Ag have been obtained by vapour quenching techniques, so far there h
ave been no reports on the Fe/Pb system. In this work, FexPb1-x films
(x = 0.10, 0.12, 0.20, 0.40, 0.42, 0.50, 0.63 and 0.70) with a thickne
ss of about 300 nm have been prepared at different deposition temperat
ures (20, 200 and 300 K) by a thermal co-evaporation technique. The in
situ Mossbauer measurements were performed to study the alloying proc
ess, the magnetic properties and the structural variation with tempera
ture. The results indicate that a solubility of 3% for Fe in Pb can be
obtained by depositing an Fe diluted film (x = 0.10) at 20 K. For the
highly Fe concentrated films, granular systems (Fe clusters) seem to
be formed at all deposition temperatures.