ZnO/CdS bilayer films have been prepared by the chemical bath deposition (C
BD) technique from a single reaction bath. The bilayer films were obtained
by using solution concentrations of 1 M for ZnSO4 and 0.1 M for CdCl2. The
pH was adjusted by the use of an ethanolamine-ammonia system. A solution 1
M of thiourea was used as the source of sulfur ions. The thickness of each
layer in the resultant film were 2 and 0.3 mum for ZnO and CdS, respectivel
y. We report here the optical and structural characterization of this ZnO/C
dS bilayer system. (C) 2001 Elsevier Science Ltd. All rights reserved.