The electrochemical polymerization of methylene green has been carried out
using cyclic voltammetry. The electrolytic solution consisted of 4 x 10(-3)
mol/L methylene green, 0.1 mol/L, NaNO3 and 1 x 10(-2) mol/L sodium tetrab
orate with pH 11.0. The temperature for polymerization is controlled at 60
degreesC. The scan potential is set between -0.2 and 1.2 V (vs, Ag/AgCl wit
h saturated KCI solution). There are an anodic peak and a cathodic peak on
the cyclic voltammogram of poly(methylene green) at pH less than or equal t
o3.8. Both peak potentials shift towards negative potentials with increasin
g pH value, and their peak currents decrease with increasing pH value. Poly
(methylene green) has a good electrochemical activity and stability in aque
ous solutions with pH less than or equal to3.8. The UV-Visible spectrum and
FTIR spectrum of poly(methylene green) are different from those of methyle
ne green.